Properties

Parylene Chemical Resistance

Parylene Chemical Resistance

diX C diX N Test Method (ASTM) Epoxies Urethanes
Density g/cm3 1.31 1.11 D1505 1.1-1.4 1.1-2.5
Refractive welcome 1.65 1.66 D542 1.55-1.61 1.50-1.60
Tensile Modulus GPa 3.2 2.4 D882
Tensile Strength psi(lb/in2) 9,800 6,800 D882 4,000-13,000 1,000-10,000
MPa 67.6 46.9 D882 28-90 7-69
Yield Strength psi(lb/in2) 9,500 7,250 D882
MPa
65.5
50.0 D882 ” width=”1″ height=”1″ /> ” width=”1″ height=”1″ />
Elongation to Break % 270 30 D882 3-6 100-1,000
Yield Elongation % 3.6 2.5 D882
Rockwell Hardness
R80 R85 D785 M80-M110
Pencil Hardness 2H 3B JIS K5600-5-4 ” width=”1″ height=”1″ /> ” width=”1″ height=”1″ />
Coefficient of Friction Static
0.29 0.25 D1894 ” width=”1″ height=”1″ /> ” width=”1″ height=”1″ />
Dynamic
0.29 0.25 D1894 ” width=”1″ height=”1″ /> ” width=”1″ height=”1″ />
Melting Point
291 420 D3417 <170
Linear Coefficient of Expansion
10-6/
30.1 69.0 45-65 100-200
Dielectric Constant 60Hz
3.10 2.65 D150 3.5-5.0 5.3-7.8
1KHz
2.83 2.65 D150 3.5-4.5 5.4-7.6
1MHz
2.87 2.67 D150 3.3-4.0 4.2-5.2
1GHz
2.81 ” width=”1″ height=”1″ /> ” width=”1″ height=”1″ /> ” width=”1″ height=”1″ />
Dissipation Factor 60Hz
0.027 0.0002 D150 0.002-0.01 0.015-0.05
1KHz
0.015 0.0002 D150 0.002-0.02 0.04-0.06
1MHz
0.014 0.0009 D150 0.03-0.05 0.05-0.07
1GHz
0.001 ” width=”1″ height=”1″ /> ” width=”1″ height=”1″ /> ” width=”1″ height=”1″ />
Dielectric Strength V/mil 6,900 7,000 D149 4,500-5,600 5,000-5,600
Volume Resistivity 23,50%RH
cm
6.9×1016
1.4×1017
D257
1012-1017
1011-1015
Surface Resistivity 23,50%RH
2.2×1015
1.0×1013
D257
1013
1014
Water Absorption 24hr % <0.1 <0.1 D570 <0.1-0.2 <0.1-1.5
Moisture Vapor Transmission 24hr,37,90%RH
gmil /100in2
0.016 1.6 F1249 1.8-2.4 2.4-8.7
Oxygen Transmission 24hr,1atm,23
cm3mil /100in2
5.38 206 D3985 5-10 200